0% found this document useful (0 votes)
514 views6 pages

Causes of Casting Defects With Remedies

This document discusses casting defects in aluminum alloy die casting. It classifies casting defects according to their root causes and describes several common metallurgical defects including porosity, sinks, and blisters. Porosity is divided into gas porosity and shrinkage porosity. Gas porosity is caused by trapped gases while shrinkage porosity results from material concentration and solidification issues. Sinks form due to insufficient metal flow filling the die cavity. Blisters occur when internal gas pressure deforms the metal surface. The document provides the causes and remedies for each of these metallurgical defects.

Uploaded by

Kavita Kale
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as DOCX, PDF, TXT or read online on Scribd
0% found this document useful (0 votes)
514 views6 pages

Causes of Casting Defects With Remedies

This document discusses casting defects in aluminum alloy die casting. It classifies casting defects according to their root causes and describes several common metallurgical defects including porosity, sinks, and blisters. Porosity is divided into gas porosity and shrinkage porosity. Gas porosity is caused by trapped gases while shrinkage porosity results from material concentration and solidification issues. Sinks form due to insufficient metal flow filling the die cavity. Blisters occur when internal gas pressure deforms the metal surface. The document provides the causes and remedies for each of these metallurgical defects.

Uploaded by

Kavita Kale
Copyright
© © All Rights Reserved
We take content rights seriously. If you suspect this is your content, claim it here.
Available Formats
Download as DOCX, PDF, TXT or read online on Scribd
You are on page 1/ 6

International Journal of Engineering Research & Technology (IJERT)

ISSN: 2278-0181
Vol. 4 Issue 11, November-2015

Causes of Casting Defects with Remedies


Rahul T Patil Veena S Metri Shubhangi S Tambore
University of Pune, University of Pune, University of Pune,
Ganeshkhind, Pune, Ganeshkhind, Pune, Ganeshkhind, Pune,
Maharashtra 411007 Maharashtra 411007 Maharashtra 411007

Abstract—- Die casting is an efficient, economical process,


offering border range of geometrically complex components and
3. METALURGICAL DEFECTS
shapes than any other manufacturing technique. But there are
defects in casting observed. In order to identify the casting
Metallurgical defects are caused by improper alloy
defect, the study is aimed in the research work. The main composition, melting temperature, defective mechanical
objective of the current paper is finding different defects in properties, internal stresses etc.
aluminum-alloy die casting and providing their remedies with
their causes. In this paper casting defects are critically discussed 3.1 POROSITY
and classified according to their root causes of occurrence.
Porosity is often used by both casting suppliers and
customers when talking about casting defects. Porosity
Keywords— Die Casting; Defects in Casting; Causes and describes the presence of voids inside casting of different
Remedies for Casting Defects size, shapes, surface constituents. Porosity can be divided
into two types.
I. INTRODUCTION
I) Gas porosity
Casting defects may be defined as characteristics which II) Shrinkage porosity
create a deficiency or imperfection to quality specification 3.1.1 Gas porosity
imposed by design and service requirement. Casting defects Gas porosity in casting is due to presence of gas
are caused by non optimized process, failure of material, which is in the form of trapped air, moisture from water
casting equipment. So the defects can be tolerated and based die lubricant, dissolved hydrogen in air. When the
repaired. In aluminum die casting the molten aluminum is pouring of metal starts the air which is present in the cavity
poured or injected into metallic die. There are many sources before pouring is compressed and the pressure rises. It forms
to cast defects and have many names. In this paper an attempt the bubbles after it has cooled.
has been made to provide al casting defects with their causes
and remedies. 3.1.1.1 Causes of gas porosity
 Speed of metal pouring is too slow .
2. CLASSIFICATION OF CASTING DEFECTS
 Presence of gas in metal.
In present paper classification of defect are based on their  Mould is too hot.
sources of defects presented in aluminum die casting. In this
classification defects are groups according to their sources.  Presence of moisture in flux.
Each of these groups includes surface and bulk defects. The  Incomplete casting.
causes and remedies of each kind of defects are explained in  Metal section is too thin.
this paper.  Overheated moulds.
 Temperature of pouring metal is low.
Classification according to the source of defects:-
3.1.1.2 Remedies
A) Metallurgical defects :
 Pouring of metal is done as rapidly as possible
Porosity, sinks, inclusion, dross, soldering.
without interaction.
B) Defects due to heat:  Use vacuum degassing. Melt the metal in vacuum.
Hot tears, cold shut, thermal fatigue.  Keep the temperature of mould low.
 Use adequate venting of moulds and cores.
C) Mechanically induced defects:
 Have sufficient metal in ladel to fill the mould.
Surface marks, bending, undercuts
 Improve the gating system.
 Modify the casting design to avoid the thin metal
section and improve runner design.
 Increase the metal pouring temperature.

IJERTV4IS1105 www.ijert.org 1
(This work is licensed under a Creative Commons Attribution 4.0 International
International Journal of Engineering Research & Technology (IJERT)
ISSN: 2278-0181
Vol. 4 Issue 11, November-2015

3.2.2 Remedies
 Use extra metal while pouring to avoid the sinks.
 Increase the gate seal time.
 Increase the injection speed to decrease viscosity
and allow more backing pressure.
 Relocate gates to problem areas.
 Increase the cooling time of metal.
 Lower the temperature of metal.
Fig 3.1 Gas porosity
3.1.2 Shrinkage Porosity
Shrinkage porosity is one of the most common
defects to rejection of aluminum casting. It can be described
as internal cracks in casting which comes from several
sources.
3.1.2.1 Causes
 Increased metal concentration at specific region.
Fig 3.3 Sinks
 Complexity in casting geometry.
3.3 Blister
 Pressure of metal is too low. In blister the thin film of small surface blows up from
 Poor gating and runner design. the part surface when the internal pressure of surface gas-
 Metal is contaminated. related porosity plastically deforms the metallic surface.
 Reduced metal volume during solidification Blister represents an example of defect of metallurgical
defect.
3.1.2.1 Remedies
 Design the die with extra tolerance. 3.3.1 Causes
 Use simple geometry in casting.  Excessively high injection rates.
 Increased metal pressure.  Pressure of gas across the surface during fill.
 Modify the getting and runner design.  Removal of parts which are at high temperature are
ejected from die.
 Use simulation software to improve runner in order
to have optimum filling of cavities.  High temperature of die surface.
 Remove the contamination, clean the metal surface. 3.3.2 Remedies
 Provide core hole in centre and offset the ribs.  Lower the injection rates.
 Use vacuum filling in casting.
 Use temperature sensors near the die.
 Lower the die surface temperature.

Fig 3.2 Shrinkage Porosity


3.2 Sinks
Sinks form when there is presence of sub-surface cavity. A
sink is depression impacting of surface of part that does not
mimic the mould surface. Sinks are often visible because they
reflects light.
3.2.1 Causes Fig 3.4 Blister
 Insufficient metal can be main reason for sinks. 3.3 Soldering
 Gate seal time is slow. Soldering is one of the main and major casting defects in
 Low injection speed. aluminum die casting process. Soldering occurs when molten
 High volumetric shrinkage. aluminum sticks the surface of die steel and remain there
 Short cooling time of metal. after the ejection of casting. Soldering occurs after just few
 High temperature of metal. casting cycle.

IJERTV4IS1105 www.ijert.org 2
(This work is licensed under a Creative Commons Attribution 4.0 International
International Journal of Engineering Research & Technology (IJERT)
ISSN: 2278-0181
Vol. 4 Issue 11, November-2015

3.3.1 Causes 3.6 Inclusions


 Poor gate design.
Inclusions are due to the presence of forging, non
 Inadequate die cooling.
metallic particles in cast metal. These are may in the form of
 Poor die surface polishing. oxides, slag, dirt, sand or nails. These inclusion can limit
 High temperature of die. mechanical properties and fatigue performance as well as
 Improper amount of iron content in alloy. lead to cosmetic defects.

3.3.2 Remedies 3.6.1 Causes


 Give more time for cooling.  Sand, dirt are not properly cleaned from moulds.
 Maintenance of die surface.  Improper gating system.
 Lower the temperature of die.  During solidification insoluble inter-metallic
 Use proper lubricant. compounds formed and segregate concentrating in
 Use proper range of iron which is between residual liquid.
0.8% to 1.1%.  Alloy additions which have not completely
dissolved in melt.
3.6.2 Remedies
 Regular cleaning of die.
 Improve gating system.
 Use clean and pour molten metal.
 Use small piece of alloying material and master
metal alloys in making up change.

Fig 3.5 Soldering


3.5 Segregation
Segregation occurs due change in chemical composition of
metal. Segregation is distinguish between two types.
Microsegregation and Macrosegregation. Microsegregation
refers to localize difference between dendrite arm. Distance
involved is about 10 to 100µm which is small for diffusion to
be significant mechanism and this is not in case of
microseggregation. Fig 3.7 Inclusion
3.6 Dross
3.5.1 Causes Dross is nothing but the metal loss. Dross in
 Local and non equilibrium composition can lead to aluminum casting contains 60.65% by weight metallic
Segregation. aluminum. Drossing is generated due to melting and holding
of aluminum. During melting, aluminum oxide( AL203) and
3.5.2 Remedy other oxides which get collected on melt surface due to
 Segregation can be removed by homogenization difference in densities.
heat treatment. 3.6.1 Causes
 Reaction result between high temp liquid aluminum
and air in melting is formation of oxides.
 Thermite reaction causes the dross.
 Higher the temperature of metal.
3.6.2 Remedies
 Lower the reaction time which reduces the
formation of dross.
 Avoid the stirring which causes the thermite reaction
Fig 3.6 Segregation and oxidation.
 Lower the temperature of the metal.

IJERTV4IS1105 www.ijert.org 3
(This work is licensed under a Creative Commons Attribution 4.0 International
International Journal of Engineering Research & Technology (IJERT)
ISSN: 2278-0181
Vol. 4 Issue 11, November-2015

Fig 3.8 Dross Fig 4.1 Crack

4 DEFECTS DUE TO THERMAL EFFECT 5 HOT TEARS


Thermal defects occurs due to pressure of thermal Hot tears is one of the main casting defect. It is due
stress in thermal origin, improper interaction of fluid and
to formation of irreversible failures of semisolid
incorrect eat removal rates.
casting. Hot tears occurs in last stage of solidification.
4.1 Cracks
Cracks are usually irregular and oxides so that 5.1.1 Causes
fracture appears dark. Crack is geometrical discontinuity in  Thermal contraction.
casting. Generally crack occurs when casting is still hot and  Abrupt section changes in casting.
contracting. Cracks can be easily seen with the naked eye and  Improper placement of gates.
other cracks are difficult to see without magnification.  Incorrect metal pouring temperature.
4.1.1 Causes  Faulty solidification methods.
 More stress localization at particular area.  Thin sections.
 High thermal concentration.
 Excessive injection forces. 5.1.2 Remedies
 Damaged die cavities.  Provide adequate fillet at junctions.
 Insufficient draft in die section.  There should be uniform thickness through out the
 Faulty die design. section.
 Shrinkage of casting in die.  Placement of gate should be accurate near the die.
4.1.2 Remedies  Use accurate metal pouring temperature.
 Proper design of casting.  Use standard solidification method.
 Use chillers in casting areas  Use minimum permissible amount of thickness.
 Give proper time for cooling of metal. Which is depends upon the casting process.
 Reduce proper pouring temperature.
 Provide feeders.
 Avoid sharp corners. Round-off the corners.
 Reduce die strength by adding saw or coal dust.

Fig 5.1 Hot tears

IJERTV4IS1105 www.ijert.org 4
(This work is licensed under a Creative Commons Attribution 4.0 International
International Journal of Engineering Research & Technology (IJERT)
ISSN: 2278-0181
Vol. 4 Issue 11, November-2015

7.1.2 Remedies
 There should be uniform thickness throughout the
section.
 Decrease the cavity fill time. Modify the gating
design.
 Decrease the flow distance by modifying the casting
design.
 Provide proper venting.
 Pouring should be done without interruption.
 Increase the temperature of metal.

Fig 5.2 Hot tears in part

6. COLD SHUT
Cold shut forms when small droplets of metal fall
into casting ,mould. Solidify and fail to combine when
remaining metal introduced to mould. Cold shut is crack with
round edges. In cold shut two different metal stream do not
forged together .

6.1.1 causes
 Lower fluidity of mould.
 Thin section of casting. Fig 7.1 Misrun in part

 Low pouring temperature of metal.


8. THERMAL FATIGUE
 Inadequate gating.
In aluminum die-casting dies are subjected to high
6.1.2 Remedies thermal stress. Thermal fatigue is due to thermal cycling
 Use different composition of metal. which shorten the life of die. A net textured of cracks forms
 Use permissible minimum thickness suitable for on the surface die.
casting process.
8.1.1 Causes
 Increase the pouring temperature.
 When the die are continuously subjected to the high
 Use proper placement of gating. temperature.
 When the edges and corners are with small radius.
 When the temperature gradient near the gate is high.

8.2 Remedies
 Cooling of die for particular period of time is
needed.
 Give permissible radius for edges and corners.
 Lower the temperature gradient near the gate.
Fig 6.1 cold shut in part

7. MISRUN
When there is incomplete filling of metal in mould
cavity and leaving unfilled portion called misrun.

7.1.1 Causes
 Thickness of section is too small.
 Too long die cavity fill time due to which entire
section is not filled before the metal solidifies.
 Long flow distance inside die cavity. Fig 8.1 Thermal defect
 Inadequate venting.
 Interruption in pouring.
 Temperature of metal is too low.

IJERTV4IS1105 www.ijert.org 5
(This work is licensed under a Creative Commons Attribution 4.0 International
International Journal of Engineering Research & Technology (IJERT)
ISSN: 2278-0181
Vol. 4 Issue 11, November-2015

9. MECHANICALLY INDUCED DEFECTS 12. CONCLUSION


Mechanically induced defects such as Surface In this research paper different casting defects are
marks, undercuts and bending occurs during ejection of studied. By referring different research papers causes and
casting and due to insufficient draft angle. Under cuts are their remedies are listed. These will help to quality control
formed due to erosion of sand by the stream of molten metal. department of casting industries for analysis of casting defect.
It shows the pattern around the gates and causes dirt in This study will definitely be helpful in improving the
casting. Bending and surface marks are caused by external productivity and yield of the casting. One of the side this
pressure loads, improper ejection methods. These defects can classification of defects helps in die caster in the stage of
be avoided by giving proper draft angle and using standard identification of the defects can be detected. Rejections of the
ejection methods and modified casting designs. casting on the basis of the casting defect should be as
minimized and all the above research is heading in the same
10. CAREFUL CONTROL OF LARGE NUMBER direction
OF VARIABLES NEEDED-
REFERENCES
• Characteristics of metals & alloys cast
• Method of casting [1] D.L cocks. “ A proposed simple qualitative classification
• Mould and die materials for die-casting”; Proc Die-casting Conference,
• Mould design Montreaux(1996)
• Process parameters- pouring, temperature, [2] ASM Handbook: Volume 15: Casting edition
9”,2008,pp629-620.
• Gating system
[3] J. Campbell, R.A hardening. “ Casting technology”, in
• Rate of cooling TAlAT 2.0ncd-rom, EAA, Brussels,2000
[4] John Gilbert Kaunfman, Elwin L. Rooy,” Aluminum
11. DESIGN MODIFICATIONS TO AVOID DEFECTS alloy casting: Properties, Processes, and application”,
ASM international,pp47-54
• Avoid sharp corners [5] R.Monroe,” porosity in casting”,AFS
• Maintain uniform cross sections Transcation,2005,pp1-29.
• Avoid shrinkage cavities [6] Defect formation in cast iron LennartElmquist School of
• Use chills to increase the rate of cooling Engineering Jönköping University, SwedenTammerfors,
Finland, November 8, 2012.
• Stagger intersecting regions
for uniform cross sections. [7] Analysis of Casting Defects and Identification of emedial
• Redesign by making parting line straight. Measures – A Diagnostic Study Dr D.N. Shivappa1, Mr
• Avoid the use of cores, if possible Rohit2, Mr. Abhijit Bhattacharya3 International Journal
• Maintain section thickness of Engineering Inventions ISSN: 2278-7461,
uniformity by redesigning www.ijeijournal.com Volume 1, Issue 6 (October2012)
• Allowances for shrinkage to be provided PP: 01-05
[8] Casting Defect Analysis using Design of Experiments
• Parting line to be along a flat (DoE) and Computer Aided Casting Simulation
plane- good at corners or edges of Technique Uday A. Dabade* and Rahul C.
casting Bhedasgaonkar,(2013) [5]. Reduction of defects in grey
• Draft to be provided cast iron castings by six sigma approach
Raguramsingh.M#1, SyathAbuthakeer.S*2 #ME Lean
• Permissible tolerances to be used Manufacturing, PSG.
• Machining allowances to be made [9] W.G WAlkington, “ Gas Porosity: A guid t corrective the
problem, North America die casting association,”1997.
• Residual stresses to be avoided
• Large flat areas to be avoided- warping due to
temperature gradients

IJERTV4IS1105 www.ijert.org 6
(This work is licensed under a Creative Commons Attribution 4.0 International

You might also like